1) How do we use silver nitrate 2 gms/ltr in palladium bath?
2) Our electroless nickel bath decomposes every day or two. Kindly suggest any kind of chemical which may stop the same.
Mr. Sunil H Jhaveri.
platers - Mumbai, Maharashtra, India
--------------------------------------------------------------------------------
A. Dear sir:
Instability of new E.N bath may be due to:
1-insufficient amount of sodium citrate (complexing agent)
2-over amounts of reducing agent (hypophosphite)
3-overheating the bath
4-unsuitable stabilizer (we use lead nitrate)
So you have the word now.
Best regards,
RAAFAT ALBENDARY
plastics electroplating - Cairo, Egypt
--------------------------------------------------------------------------------
A. Dear sir:
1-Sorry because I forgot the first part of the question.
2-If you insist to use silver nitrate in activation bath it is not recommended to put it in palladium bath; otherwise it will precipitate as silver chloride
3- The formula for using silver in activation bath is: silver nitrate:2 gm/l sodium borates: 20 gm/l
4-In this case you have to use electroless copper or special type of electroless nickel
Thanks and best regards,
RAAFAT ALBENDARY
plastics electroplating - Cairo, Egypt
Electroless Plating
by Mallory & Hajdu
--------------------------------------------------------------------------------
Q. Raafat, what is your formula for an electroless nickel bath? Also, what is the cycle used to activate nonconductors for plating using silver nitrate? I have always used tin-palladium systems. I thank you in advance.
Michael Brewington
- Salisbury, Maryland, USA
--------------------------------------------------------------------------------
A. Michael, I have no private formula for electroless nickel but it's my understanding that:
1-The activation metal [Ag ,Pd] it is very important to know the relation between the metal and the reducing agent in the electroless bath. Example, silver is not catalytic to the electroless nickel when hypophosphite is not catalytic to initiate or start the reaction but in borane {NaHB, Di methyl hydrogenborane [DMHB]} it will be catalytic. So the reducing agent plays a very important role.
2-The plating procedure for non conductors using silver in activation is as follows: 1-degreasing 2-etching 3-activation 4-electroless plating 5-electroplating.
Thanks and best regards,
RAAFAT ALBENDARY
PLASTICS ELECTROPLATING - Cairo, EGYPT
--------------------------------------------------------------------------------
Q. Dear sir,
Is it necessary to sensitize with SnCl2 before activation with AgNO3/borate? And it will explode like fulminate of silver?
Best regard,
Prasarn Hutpattanasilp
- Samutsakorn Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir,
No need for sensitizing with [SnCL2] and the solution is very stable and there is no chance for explosive action.
Thanks and best regards,
RAAFAT ALBENDARY
Plastics Electroplating - Cairo, Egypt
--------------------------------------------------------------------------------
Q. Dear sir,
Do you have recommended safety procedure for using AgNO3/borate without explosion? What kind of borate used, sodium borate (sodium metaborate tetrahydrate), sodium perborate, sodium tetraborate decahydrate, sodium tetraborate anhydrous?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir, sodium borate is borax, which has the formula of [Na2B4O7.10H2O]. The activation cycle is simple:
1-etching
2-neutralization
3-activation in silver bath
4-rinsing [distilled water]
5-rinsing
6-electroless copper
7-electroplating
Thanks and best regards,
Raafat Albendary
Plastics Electroplating - Cairo, Egypt
Electroless Copper and Nickel-Phosphorous Plating
--------------------------------------------------------------------------------
Q. Dear Raafat ,
It is sodium tetraborate decahydrate, is that right?
What type of reducing agent use in electroless copper (formaldehyde type can do this job)? And if sensitizing (SnCl2/HCl) step is add it will enhance activity?
Best regard,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir,
1-Yes it is tetra borate deca hydrate.
2-Formaldhyde type is OK.
3-Never use HCl before any silver borate because there will be some traces of [Cl-] ions which will precipitate silver as silver chloride and that spoils the solution. And simply no need for that because [HCHO] will reduce silver [Ag+1] to [Ag0] which is able to initiate the electroless reaction.
Thanks,
RAAFAT ALBENDARY
- CAIRO, EGYPT
--------------------------------------------------------------------------------
Q. Dear Raafat,
Can you recommend the process to promote absorption of silver/borate to plastic after etching to enhance the activity in electroless copper and/or improve adhesion of metal to plastic?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
Dear sir,
I don't understand your response.
Best regards
RAAFAT ALBENDARY
- Cairo, Egypt
--------------------------------------------------------------------------------
Dear Raffat,
I mean in the conventional process when use fulminate silver as activator must use sensitizer step (SnCl2/HCl) to enhance absorption of fulminate silver (in fact reduce Ag(I) to Ag(0) ) and go to electroless copper. So if the sensitizing step is omitted the Ag species that absorbed on the plastic is Ag(1) and go to electroless copper (formaldehyde in electroless will reduce Ag(I) to Ag (0) ) so the activity will slow (covering time)? So I will ask that it has any process chemical to promote absorption instead of SnCl2/HCl or not?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir, we talk too much on this subject. Why don't you try to test our claims and tell me the results.
best regards,
RAAFAT ALBENDARY
PLASTICS ELECTROPLATING - CAIRO-EGYPT
--------------------------------------------------------------------------------
Q. Dear Raafat,
I have tried your formula and found.
1. On make up the solution go brownish and a lot white precipitate (maybe from commercial grade borate? We use DI water).
2. After make up the solution has brown colloidal dispersion throughout the solution.
3. The activity is so slow in electroless copper and we have skip plating.
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir,
Try to get ready-made silver borate because what you mentioned mean that [SILVER TRACES] found in the solution when you made activation.
Thanks and best regards,
RAAFAT ALBENDARY
- CAIRO, Egypt
--------------------------------------------------------------------------------
Q. Dear Raafat,
I've been watching this conversation with some interest and have a couple of questions for you.
1 Does the silver activator offer any advantages over conventional tin/palladium activators?
2 How tolerant is it to different types of plating grade ABS?
3 How closely does the process have to be controlled to prevent skip plating or at the other end of the scale rack plate up?
4 How would the toxicity of this process compare to a tin/ palladium process?
Kind regards,
Tim Strickland
- Auckland , New Zealand
--------------------------------------------------------------------------------
Q. DEAR RAAFAT,
I NEED YOUR HELP. WHAT IS YOUR ELECTROLESS COPPER FORMULATION. I'M WORKING ELECTROLESS NICKEL. IT CONTAINS SODIUM CITRATE, NICKEL CHLORIDE, SODIUM HYPOPHOSPITE, AMMONIUM CHLORIDE. MY ACTIVATOR IS PALLADIUM. BUT IT'S TOO EXPENSIVE. CAN I WORK SILVER NITRATE/BORANE SYSTEM WITH THIS ELECTROLESS NICKEL FORMULATION?
BEST REGARDS,
MURAT CETIN
- Izmir, Turkey
--------------------------------------------------------------------------------
A. Dear friends,
Sorry for lateness.
For first friend:
what silver activator added to us:
1-it is not expensive
2-it gives us ability to plate other kinds of plastics rather than ABS [polyester-p.v.c p.s high impact] etc.
3-not sensitive to changes of pH
4-it is very stable
5-no need for sensitizing with [SnCl2]
For second friend:
My formula [actually it is not my invention] is:
copper sulphate 5 gm/L
triethanol amin 10 gm/L
formaldehyde 20 ml/L
pH>12 [adjusted with NaOH]
temp. room
You couldn't use this activator with E.N because silver is not catalytic to nickel when hypophosphite is the reducing agent
Thanks & best regards,
RAAFAT ALBENDARY
PLASTICS ELECTROPLATING - CAIRO, EGYPT
--------------------------------------------------------------------------------
Q. Dear Raafat,
I have found interesting for your electroless copper solution. You use commercial TEA (99%) instead of Na.K.tatrate that right? TEA can be used as stabilizer?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
Q. Dear Raafat.
Thank you for your answer. Is necessary to stabilizer like thiourea, lead acetate vs? And how do you control this solution? Are you using air agitation and filtration? Have a good religious.
Best Regards,
MURAT CETIN
- Izmir, Turkey
1) How do we use silver nitrate 2 gms/ltr in palladium bath?
2) Our electroless nickel bath decomposes every day or two. Kindly suggest any kind of chemical which may stop the same.
Mr. Sunil H Jhaveri.
platers - Mumbai, Maharashtra, India
--------------------------------------------------------------------------------
A. Dear sir:
Instability of new E.N bath may be due to:
1-insufficient amount of sodium citrate (complexing agent)
2-over amounts of reducing agent (hypophosphite)
3-overheating the bath
4-unsuitable stabilizer (we use lead nitrate)
So you have the word now.
Best regards,
RAAFAT ALBENDARY
plastics electroplating - Cairo, Egypt
--------------------------------------------------------------------------------
A. Dear sir:
1-Sorry because I forgot the first part of the question.
2-If you insist to use silver nitrate in activation bath it is not recommended to put it in palladium bath; otherwise it will precipitate as silver chloride
3- The formula for using silver in activation bath is: silver nitrate:2 gm/l sodium borates: 20 gm/l
4-In this case you have to use electroless copper or special type of electroless nickel
Thanks and best regards,
RAAFAT ALBENDARY
plastics electroplating - Cairo, Egypt
Electroless Plating
by Mallory & Hajdu
--------------------------------------------------------------------------------
Q. Raafat, what is your formula for an electroless nickel bath? Also, what is the cycle used to activate nonconductors for plating using silver nitrate? I have always used tin-palladium systems. I thank you in advance.
Michael Brewington
- Salisbury, Maryland, USA
--------------------------------------------------------------------------------
A. Michael, I have no private formula for electroless nickel but it's my understanding that:
1-The activation metal [Ag ,Pd] it is very important to know the relation between the metal and the reducing agent in the electroless bath. Example, silver is not catalytic to the electroless nickel when hypophosphite is not catalytic to initiate or start the reaction but in borane {NaHB, Di methyl hydrogenborane [DMHB]} it will be catalytic. So the reducing agent plays a very important role.
2-The plating procedure for non conductors using silver in activation is as follows: 1-degreasing 2-etching 3-activation 4-electroless plating 5-electroplating.
Thanks and best regards,
RAAFAT ALBENDARY
PLASTICS ELECTROPLATING - Cairo, EGYPT
--------------------------------------------------------------------------------
Q. Dear sir,
Is it necessary to sensitize with SnCl2 before activation with AgNO3/borate? And it will explode like fulminate of silver?
Best regard,
Prasarn Hutpattanasilp
- Samutsakorn Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir,
No need for sensitizing with [SnCL2] and the solution is very stable and there is no chance for explosive action.
Thanks and best regards,
RAAFAT ALBENDARY
Plastics Electroplating - Cairo, Egypt
--------------------------------------------------------------------------------
Q. Dear sir,
Do you have recommended safety procedure for using AgNO3/borate without explosion? What kind of borate used, sodium borate (sodium metaborate tetrahydrate), sodium perborate, sodium tetraborate decahydrate, sodium tetraborate anhydrous?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir, sodium borate is borax, which has the formula of [Na2B4O7.10H2O]. The activation cycle is simple:
1-etching
2-neutralization
3-activation in silver bath
4-rinsing [distilled water]
5-rinsing
6-electroless copper
7-electroplating
Thanks and best regards,
Raafat Albendary
Plastics Electroplating - Cairo, Egypt
Electroless Copper and Nickel-Phosphorous Plating
--------------------------------------------------------------------------------
Q. Dear Raafat ,
It is sodium tetraborate decahydrate, is that right?
What type of reducing agent use in electroless copper (formaldehyde type can do this job)? And if sensitizing (SnCl2/HCl) step is add it will enhance activity?
Best regard,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir,
1-Yes it is tetra borate deca hydrate.
2-Formaldhyde type is OK.
3-Never use HCl before any silver borate because there will be some traces of [Cl-] ions which will precipitate silver as silver chloride and that spoils the solution. And simply no need for that because [HCHO] will reduce silver [Ag+1] to [Ag0] which is able to initiate the electroless reaction.
Thanks,
RAAFAT ALBENDARY
- CAIRO, EGYPT
--------------------------------------------------------------------------------
Q. Dear Raafat,
Can you recommend the process to promote absorption of silver/borate to plastic after etching to enhance the activity in electroless copper and/or improve adhesion of metal to plastic?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
Dear sir,
I don't understand your response.
Best regards
RAAFAT ALBENDARY
- Cairo, Egypt
--------------------------------------------------------------------------------
Dear Raffat,
I mean in the conventional process when use fulminate silver as activator must use sensitizer step (SnCl2/HCl) to enhance absorption of fulminate silver (in fact reduce Ag(I) to Ag(0) ) and go to electroless copper. So if the sensitizing step is omitted the Ag species that absorbed on the plastic is Ag(1) and go to electroless copper (formaldehyde in electroless will reduce Ag(I) to Ag (0) ) so the activity will slow (covering time)? So I will ask that it has any process chemical to promote absorption instead of SnCl2/HCl or not?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir, we talk too much on this subject. Why don't you try to test our claims and tell me the results.
best regards,
RAAFAT ALBENDARY
PLASTICS ELECTROPLATING - CAIRO-EGYPT
--------------------------------------------------------------------------------
Q. Dear Raafat,
I have tried your formula and found.
1. On make up the solution go brownish and a lot white precipitate (maybe from commercial grade borate? We use DI water).
2. After make up the solution has brown colloidal dispersion throughout the solution.
3. The activity is so slow in electroless copper and we have skip plating.
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
A. Dear sir,
Try to get ready-made silver borate because what you mentioned mean that [SILVER TRACES] found in the solution when you made activation.
Thanks and best regards,
RAAFAT ALBENDARY
- CAIRO, Egypt
--------------------------------------------------------------------------------
Q. Dear Raafat,
I've been watching this conversation with some interest and have a couple of questions for you.
1 Does the silver activator offer any advantages over conventional tin/palladium activators?
2 How tolerant is it to different types of plating grade ABS?
3 How closely does the process have to be controlled to prevent skip plating or at the other end of the scale rack plate up?
4 How would the toxicity of this process compare to a tin/ palladium process?
Kind regards,
Tim Strickland
- Auckland , New Zealand
--------------------------------------------------------------------------------
Q. DEAR RAAFAT,
I NEED YOUR HELP. WHAT IS YOUR ELECTROLESS COPPER FORMULATION. I'M WORKING ELECTROLESS NICKEL. IT CONTAINS SODIUM CITRATE, NICKEL CHLORIDE, SODIUM HYPOPHOSPITE, AMMONIUM CHLORIDE. MY ACTIVATOR IS PALLADIUM. BUT IT'S TOO EXPENSIVE. CAN I WORK SILVER NITRATE/BORANE SYSTEM WITH THIS ELECTROLESS NICKEL FORMULATION?
BEST REGARDS,
MURAT CETIN
- Izmir, Turkey
--------------------------------------------------------------------------------
A. Dear friends,
Sorry for lateness.
For first friend:
what silver activator added to us:
1-it is not expensive
2-it gives us ability to plate other kinds of plastics rather than ABS [polyester-p.v.c p.s high impact] etc.
3-not sensitive to changes of pH
4-it is very stable
5-no need for sensitizing with [SnCl2]
For second friend:
My formula [actually it is not my invention] is:
copper sulphate 5 gm/L
triethanol amin 10 gm/L
formaldehyde 20 ml/L
pH>12 [adjusted with NaOH]
temp. room
You couldn't use this activator with E.N because silver is not catalytic to nickel when hypophosphite is the reducing agent
Thanks & best regards,
RAAFAT ALBENDARY
PLASTICS ELECTROPLATING - CAIRO, EGYPT
--------------------------------------------------------------------------------
Q. Dear Raafat,
I have found interesting for your electroless copper solution. You use commercial TEA (99%) instead of Na.K.tatrate that right? TEA can be used as stabilizer?
Best regards,
Prasarn Hutpattanasilp
- Samutsakorn, Center, Thailand
--------------------------------------------------------------------------------
Q. Dear Raafat.
Thank you for your answer. Is necessary to stabilizer like thiourea, lead acetate vs? And how do you control this solution? Are you using air agitation and filtration? Have a good religious.
Best Regards,
MURAT CETIN
- Izmir, Turkey
การแปล กรุณารอสักครู่..
1 ) เราจะใช้ไนเตรตเงิน 2 กรัม / ลิตรในน้ำอาบ
2 ) นิกเกิลแบบไม่มีไฟฟ้าสลายตัวเราอาบทุกวันหรือสอง กรุณาแนะนำชนิดของสารเคมีซึ่งอาจหยุดเหมือนกัน
นาย Sunil H jhaveri .
platers - มุมไบ , Maharashtra , อินเดีย --------------------------------------------------------------------------------
. . Dear Sir : ความไม่แน่นอนของ N อาบใหม่ อาจเป็นเพราะ :
จำนวน 1-insufficient โซเดียมซิเทรต ( ในตัวแทน )
2-over ปริมาณ reducing agent ( Hypophosphite )
3-overheating อาบน้ำ
4-unsuitable โคลง ( เราใช้ตะกั่วไนเตรท )
ดังนั้นคุณมีพระวจนะตอนนี้ นับถือ
raafat albendary พลาสติกชุบ - ไคโร , อียิปต์ --------------------------------------------------------------------------------
. . ที่รัก ครับ
:1-sorry เพราะฉันลืมส่วนแรกของคำถาม
2-if คุณยืนยันที่จะใช้ไนเตรตเงินกระตุ้นนํ้าจะไม่แนะนำให้ใส่ในน้ำอาบ มิฉะนั้นมันจะตกตะกอนเป็นซิลเวอร์คลอไรด์
3 - สูตรสำหรับใช้ในการอาบเงิน : ไนเตรตเงิน : 2 : 20 กรัม / ลิตรโซเดียมบอเรตกรัม / ลิตร
4-in กรณีนี้คุณต้องใช้ชนิดพิเศษของอุตสาหกรรมการผลิตทองแดงหรือนิกเกิลแบบไม่มีไฟฟ้า
ขอขอบคุณและขอแสดงความนับถือ
raafat albendary
พลาสติกชุบ - ไคโร , อียิปต์ชุบไฟฟ้า
โดย Mallory & hajdu
Q -------------------------------------------------------------------------------- raafat อะไรเป็นสูตรของคุณสำหรับการอาบ นิกเกิลแบบไม่มีไฟฟ้า ? นอกจากนี้นี่เป็นวงจรที่ใช้เพื่อเปิดใช้งานสำหรับการใช้ไนเตรท nonconductors ชุบเงิน ผมมักจะใช้ระบบแพลเลเดียมดีบุก ผมขอขอบคุณล่วงหน้า
ไมเคิล brewington
- ซาลิสบิวรี , Maryland , USA
-------------------------------------------------------------------------------- . ไมเคิล ผมไม่มีส่วนสูตรสำหรับนิกเกิลแบบไม่มีไฟฟ้า แต่ก็เข้าใจว่า
1-the กระตุ้นโลหะ [ AG , PD ] มันเป็นสิ่งสำคัญมากที่จะรู้ว่าความสัมพันธ์ระหว่างโลหะและลดเจ้าหน้าที่อาบน้ำแบบไม่มีไฟฟ้า . เช่น เงินไม่ต้องเร่งปฏิกิริยานิกเกิลแบบไม่มีไฟฟ้าเมื่อ Hypophosphite ไม่ใช่ตัวเร่งปฏิกิริยาให้เริ่มต้นหรือเริ่มต้นปฏิกิริยา แต่ในไดเมทิล hydrogenborane NAHB โบเรน { , [ dmhb ] } จะเร่งปฏิกิริยา ดังนั้นการลดเจ้าหน้าที่มีบทบาทสำคัญมาก
2 - ขั้นตอนไม่ชุบไฟฟ้าโดยใช้เงินในการเปิดใช้งานมีดังนี้ 1-degreasing 2-etching 3-activation 4-electroless ชุบ 5-electroplating ขอบใจนะ
และขอแสดงความนับถือ
raafat albendary
พลาสติกชุบ - ไคโร , อียิปต์ --------------------------------------------------------------------------------
Q Dear Sir ,มันจำเป็นต้องความรู้สึกไวกับ sncl2 ก่อนการกระตุ้นด้วย agno3 / บอเรต ? และมันจะระเบิดเหมือนวิพากษ์ของเงิน ? เรื่องดีที่สุด
- ศูนย์ประสาน hutpattanasilp จังหวัดสมุทรสาครประเทศไทย
-------------------------------------------------------------------------------- เซอร์รัก
,ไม่ต้อง sensitizing ด้วย [ sncl2 ] และโซลูชั่นมั่นคงมาก และไม่มีโอกาสสำหรับการกระทำระเบิด ขอบคุณ
และขอแสดงความนับถือ
raafat albendary
พลาสติกชุบ - ไคโร , อียิปต์ --------------------------------------------------------------------------------
Q Dear Sir , คุณมีขั้นตอนที่แนะนำเพื่อความปลอดภัยในการใช้ agno3 / บอเรตโดยไม่มีการระเบิดชนิดของบอเรทใช้ โซเดียมบอเรต ( Sodium metaborate โมลิบเดตเตตระไฮเดรต ) , โซเดียม perborate โซเดียมเตตราบอเรต decahydrate โซเดียมเตตราบอเรต , รัส ? ขอแสดงความนับถือ
+ hutpattanasilp
- สมุทรสาคร , ศูนย์ , ประเทศไทย
-------------------------------------------------------------------------------- . Dear Sir , โซเดียมบอเรต คือ สารบอแรกซ์ ซึ่งมีสูตร [ na2b4o7.10h2o ]วงจรใช้งานง่าย :
3-activation 1-etching 2-neutralization สีเงินอาบ 4-rinsing
[ ]
6-electroless น้ำกลั่น 5-rinsing 7-electroplating ทองแดง
ขอขอบคุณและขอแสดงความนับถือ
raafat albendary
พลาสติกชุบ - ไคโร , อียิปต์
อุตสาหกรรมการผลิตทองแดงและนิกเกิลชุบฟอสฟอรัส
--------------------------------------------------------------------------------
Qraafat
ที่รัก , มันเป็นโซเดียมเตตราบอเรต decahydrate ใช่ไหม ?
สิ่งที่ประเภทของปริมาณสารใช้ในอุตสาหกรรมการผลิตทองแดง ( ประเภทฟอร์มาลดีไฮด์สามารถทำงานนี้ได้ ) และถ้า sensitizing ( sncl2 / HCl ) ขั้นตอนจะเพิ่มก็เพิ่มกิจกรรม เรื่องดีที่สุด
+ hutpattanasilp
- สมุทรสาคร , ศูนย์ , ไทย --------------------------------------------------------------------------------
. . ที่รัก
1-yes เป็น Tetra บอเรตเดคาไฮเดรต .
ประเภท 2-formaldhyde OK
3-never ใช้ HCl ก่อนที่เงินบอเรต เพราะจะต้องมีร่องรอยของ [ CL ] - ไอออน ซึ่งจะทำให้การเงินเป็นเงินคลอไรด์ และริบโซลูชั่น และก็ไม่ต้อง เพราะ [ hcho ] จะลดเงิน [ 1 ] [ 1 ] ซึ่งเป็น ag0 สามารถเริ่มต้นปฏิกิริยาอุตสาหกรรมการผลิต
ขอบคุณ
raafat albendary
- ไคโรอียิปต์
--------------------------------------------------------------------------------
Q
raafat ที่รัก , คุณสามารถแนะนำขั้นตอนการส่งเสริมการดูดซึมของเงิน / บอเรตพลาสติกหลังจากการเพิ่มกิจกรรมในอุตสาหกรรมการผลิตทองแดงและ / หรือปรับปรุงการยึดติดของโลหะกับพลาสติก ? ขอแสดงความนับถือ
+ hutpattanasilp
- สมุทรสาคร , ศูนย์ , ประเทศไทย
--------------------------------------------------------------------------------
ท่านที่รัก
ผมไม่ค่อยเข้าใจคำตอบของคุณ
นับถือ
raafat albendary
- ไคโร , อียิปต์ --------------------------------------------------------------------------------
raffat ที่รัก ,ผมหมายถึงในกระบวนการปกติเมื่อใช้วิพากษ์สีเงินเป็น activator ต้องใช้ทุกขั้นตอน ( sncl2 / HCl ) เพื่อเพิ่มการดูดซึมของวิพากษ์ซิลเวอร์ ( ในความเป็นจริงลด AG ( ฉัน ) AG ( 0 ) และไปแบบไม่มีไฟฟ้าทองแดงดังนั้น ถ้า sensitizing ขั้นตอนจะถูกตัดออกโดยชนิดที่ดูดซึมในพลาสติก เอจี ( 1 ) และไปแบบไม่มีไฟฟ้าทองแดง ( ฟอร์มาลดีไฮด์ในอุตสาหกรรมการผลิตจะลด AG ( ฉัน ) AG ( 0 ) ดังนั้นกิจกรรมจะช้า ( ครอบคลุมครั้ง ) ดังนั้น ผมจะถามว่ามันมีกระบวนการทางเคมีใด ๆเพื่อส่งเสริมการดูดซึมแทน sncl2 / hcl หรือไม่ ? ขอแสดงความนับถือ
+ hutpattanasilp
- สมุทรสาคร , ศูนย์ , ประเทศไทย
--------------------------------------------------------------------------------
. Dear Sir , เราพูดมากเกี่ยวกับเรื่องนี้ ทำไมคุณไม่ลองทดสอบการเรียกร้องของเรา และบอกผล นับถือ
raafat albendary พลาสติกชุบ - cairo-egypt
--------------------------------------------------------------------------------
Q
raafat ที่รัก ,ฉันได้ลองสูตรของคุณและพบ
1 แต่งหน้าวิธีไปสีน้ำตาลและสีขาวอยู่มาก ( อาจจะจากเกรดบอเรต ? เราใช้น้ำ DI )
2 หลังจากสร้างโซลูชันมีสีน้ำตาลกระจายทั่วสารละลายคอลลอยด์ .
3 กิจกรรมที่ช้ามากในอุตสาหกรรมการผลิตทองแดงและเราได้ข้ามการชุบ ขอแสดงความนับถือ
+ hutpattanasilp
- สมุทรสาคร , ศูนย์ , ประเทศไทย
--------------------------------------------------------------------------------
. . ท่านที่รัก
ลองบอเรตเงินสำเร็จรูป เพราะสิ่งที่คุณกล่าวหมายถึง ร่องรอย [ ซิลเวอร์ ] พบในการแก้ปัญหา เมื่อคุณได้เปิดใช้งาน ขอบคุณ
และขอแสดงความนับถือ
raafat albendary
- ไคโร , อียิปต์ --------------------------------------------------------------------------------
raafat คิวที่รัก ,ผมเคยดูเรื่องนี้กับบางอย่างที่น่าสนใจ และมีคู่ของคำถามสำหรับคุณ
1 จะกระตุ้นเงินเสนอข้อได้เปรียบเหนือธรรมดาดีบุก / แพลเลเดียมกระตุ้น ?
2 วิธีใจกว้างเป็นชนิดที่แตกต่างกันของชุบเกรดจาก
3 วิธีการอย่างใกล้ชิดแล้ว กระบวนการต้องได้รับการควบคุมเพื่อป้องกันไม่ให้ข้ามชุบหรือที่ส่วนอื่น ๆของขนาดแผ่นชั้น ?
4 จะมีความเป็นพิษของกระบวนการนี้เปรียบเทียบกับกระบวนการดีบุก / แพลเลเดียม ?
เกี่ยวกับชนิด
ทิม Strickland
- โอ๊คแลนด์ นิวซีแลนด์ --------------------------------------------------------------------------------
raafat คิวที่รัก , ฉันต้องการความช่วยเหลือของคุณ อะไรคือสูตรของคุณทองแดงแบบไม่มีไฟฟ้า . ผมทำงาน นิกเกิลแบบไม่มีไฟฟ้า . ประกอบด้วยโซเดียมซิเตรต hypophospite นิเกิลคลอไรด์ โซเดียม ,แอมโมเนียมคลอไรด์ การกระทำของฉันคือแพลเลเดียม แต่มันแพงเกินไป ฉันสามารถทำงานระบบไนเตรท / โบเรนเงิน นิกเกิลแบบไม่มีไฟฟ้าใช้นี้ ? ขอแสดงความนับถือ
- Murat เซติน Izmir , ตุรกี --------------------------------------------------------------------------------
. . เพื่อน ๆ ที่รัก
ขอโทษที่ล่าช้า
สำหรับเพื่อนคนแรก :
อะไรเงินกระตุ้นเพิ่มเรา
1-it ไม่แพง2-it ให้ในแผ่นชนิดอื่น ๆของพลาสติก ABS PS มากกว่า [ polyester-p.v.c ผลกระทบสูง ] ฯลฯ
3-not ไวต่อการเปลี่ยนแปลงของ pH
4-it ต้อง 5-no เสถียรภาพมากสำหรับ sensitizing
[ ]
sncl2 เพื่อนที่สอง :
[ สูตรของฉันจริง ๆไม่ใช่ ] การประดิษฐ์ของฉัน :
5 ทองแดงซัลเฟต กรัม / ลิตร
triethanol อามิน 10 กรัม / ลิตร ปริมาณ 20 ml / l
M > 12 [ ปรับด้วย NaOH ]
ชั่วคราว ห้อง
คุณไม่สามารถใช้ Activator กับ E . N เพราะเงินไม่ได้เป็นตัวเร่งปฏิกิริยานิกเกิลเมื่อ Hypophosphite เป็น reducing agent
ขอบคุณ&ขอแสดงความนับถือ
raafat albendary
พลาสติกชุบ - ไคโร , อียิปต์ --------------------------------------------------------------------------------
Q
raafat ที่รัก , ฉันได้พบที่น่าสนใจสำหรับโซลูชั่นของคุณทองแดงแบบไม่มีไฟฟ้า .คุณใช้ชาพาณิชย์ ( 99% ) แทน na.k.tatrate ใช่ไหม ? ชาสามารถใช้เป็นโคลง ? ขอแสดงความนับถือ
+ hutpattanasilp
- สมุทรสาคร , ศูนย์ , ประเทศไทย
Q -------------------------------------------------------------------------------- ที่รัก raafat .
ขอบคุณสำหรับคำตอบครับ ต้องโคลงเช่น Thiourea , ตะกั่วอะซิเตท VS ? และวิธีที่คุณสามารถควบคุมวิธีการแก้ปัญหานี้ ?คุณจะใช้มาก อากาศ และกรอง ? มีศาสนา นับถือ
,
Murat เซติน
- Izmir , ตุรกี
การแปล กรุณารอสักครู่..